Objectives. Third-body wear is believed to be one trigger for adverse results
with metal-on-metal (MOM) bearings. Impingement and subluxation
may release metal particles from MOM replacements. We therefore
challenged MOM bearings with relevant debris types of cobalt–chrome
alloy (CoCr), titanium alloy (Ti6Al4V) and polymethylmethacrylate
bone cement (PMMA). Methods. Cement flakes (PMMA), CoCr and Ti6Al4V particles (size range
5 µm to 400 µm) were run in a MOM wear simulation. Debris allotments
(5 mg) were inserted at ten intervals during the five million cycle
(5 Mc) test. . Results. In a clean test phase (0 Mc to 0.8 Mc), lubricants retained their
yellow colour. Addition of metal particles at 0.8 Mc turned lubricants
black within the first hour of the test and remained so for the
duration, while PMMA particles did not change the colour of the
lubricant. Rates of wear with PMMA, CoCr and Ti6Al4V debris averaged
0.3 mm. 3. /Mc, 4.1Â mm. 3. /Mc and 6.4 mm. 3. /Mc,
respectively. . Conclusions. Metal particles turned