INTRODUCTION

Hip wear simulator test results could be affected by many non-bearing related factors such as fixation surface conditions, equipment calibration and component set-up. In an effort to improve the accuracy, reliability and repeatability of hip simulator test, a quality management system has been established at the IDC hip tribology laboratory, which has been accredited by UKAS (United Kingdom Accreditation Service) in accordance with the recognised international standard ISO17025. This study demonstrates that under well-controlled laboratory and testing conditions, satisfactory repeatability can be achieved during hip simulator studies.

METHODS

Between 2008 to 2010, ten 50 mm Birmingham Hip Resurfacing (BHR) devices were tested by the IDC tribology laboratory using two ProSim hip wear simulators in three different tests (T1, T2 and T3). All tests were performed following the same IDC testing protocols at 1 Hz frequency for 5 million cycles (Mc) or until after a steady state was reached. Paul type stance phase loadings with a maximum load of 3 kN and a swing phase load of 0.3 kN was used. The flexion and extension angles were 30 and 15 degree. The internal/external rotation angel was ±10 degree. Wear was measured gravimetrically using an analytical balance (Mettler, Toledo xp504) with an accuracy of 0.1 mg.


Orthopaedic Proceedings
Vol. 94-B, Issue SUPP_XXXVII | Pages 239 - 239
1 Sep 2012
Hussain A Hussain A Kamali A Li C Pamu J Ashton R
Full Access

INTRODUCTION

Analysis of retrieved ceramic components have shown areas of localized ‘stripe wear’, which have been attributed to joint laxity and/or impingement resulting in subluxation of the head, causing wear on the edge of the cup. Studies have been conducted into the effects of mild subluxation, however few in vitro tests have looked at severe subluxation. The aim of this study was to develop a more clinically relevant subluxation protocol.

MATERIALS & METHODS

Seven (Subluxation n=4; standard test n=3) of 36mm Biolox Forte (R3, Smith & Nephew) ceramic devices were tested for 0.5m cycles (mc). Two of the subluxed joints were further tested to 1 Mc. The devices were subjected to subluxation under standard testing conditions. The flex/ext was 30° and 15° respectively, with internal/external rotation of ±10°. The force was Paul type stance phase loading with a maximum load of 3 kN, and a standard ISO swing phase load of 0.3 kN at 1 Hz.

The test was conducted on a ProSim hip joint wear simulator (SimSol, UK). The simulator is equipped with a novel mechanism to achieve translation of the head, to achieve subluxation. During the ISO swing phase load of 0.3kN, a controlled lateral force required for the translation of the head is applied by a cam mechanism, head retraction then occurs during heel strike.

The lubricant used was new born calf serum diluted with de-ionised water to achieve average protein concentration of 20 g/l, with 0.2 wt % concentration NaN3, and changed every 250k cycles. Measurements have been taken at 0.5 & 1 mc stages.