Advertisement for orthosearch.org.uk
Results 1 - 6 of 6
Results per page:
Applied filters
Content I can access

Include Proceedings
Dates
Year From

Year To
Orthopaedic Proceedings
Vol. 94-B, Issue SUPP_XXXVII | Pages 145 - 145
1 Sep 2012
Tayton E Kalra S Briscoe A Aarvold A Smith J Lanham S Fahmy S Howdle S Shakesheff K Dunlop D Oreffo R
Full Access

Background

Impaction bone grafting with milled human allograft is the gold standard for replacing lost bone stock during revision hip surgery. Problems surrounding the use of allograft include cost, availability, disease transmission and stem subsidence (usually due to shear failure of the surrounding allograft). Aims. To investigate various polymers for use as substitute allograft. The ideal graft would be a composite with similar mechanical characteristics as allograft, and with the ability to form de novo bone.

Methods

High and low molecular weight (MW) forms of three different polymers (polylactic acid (PLA), poly (lactic-co-glycolic) acid (PLGA) and polycaprolactone (PCL)) were milled, impacted into discs, and then tested in a custom built shear testing rig, and compared to allograft. A second stage of the experiment involved the addition of skeletal stem cells (SSC) to each of the milled polymers, impaction, 8 days incubation, and then tests for cell viability and number, via fluorostaining and biochemical (WST-1, DNA) assays.


Orthopaedic Proceedings
Vol. 94-B, Issue SUPP_XXXIX | Pages 212 - 212
1 Sep 2012
Tayton E Purcell M Briscoe A Kalra S Aarvold A Smith J Fahmy S Shakesheff K Howdle S Dunlop D Oreffo R
Full Access

Aims

Disease transmission, availability and economic costs of allograft have resulted in significant efforts into finding an allograft alternative for use in impaction bone grafting (IBG). Biotechnology offers the combination of skeletal stem cells (SSC) with biodegradable polymers as a potential solution. Recently polymers have been identified with both structural strength and SSC compatibility that offer the potential for clinical translation.

The aim of this study was to assess whether increasing the porosity of one such polymer via super critical CO2 fluid foaming (SCF) enhanced the mechanical and cellular compatibility characteristics for use as an osteogenic alternative to allograft in IBG.

Methods

High molecular weight PLA scaffolds were produced via traditional (solid block) and SCF (porous) techniques, and the differences characterised using scanning electron microscopy (SEM). The polymers were milled, impacted, and mechanical comparison between traditional vs SCD created scaffolds and allograft controls was made using a custom shear testing rig, as well as a novel agitation test to assess cohesion. Cellular compatibility tests for cell number, viability and osteogenic differentiation using WST-1 assays, fluorostaining and ALP assays were determined following 14 day culture with SSC's.


Orthopaedic Proceedings
Vol. 94-B, Issue SUPP_XXXIX | Pages 211 - 211
1 Sep 2012
Tayton E Fahmy S Aarvold A Smith J Kalra S Briscoe A Shakesheff K Howdle S Dunlop D Oreffo R
Full Access

Aims

Impaction bone grafting with milled human allograft is the gold standard for replacing lost bone stock during revision hip surgery. Problems surrounding the use of allograft include cost, availability, disease transmission and stem subsidence (usually due to shear failure of the surrounding allograft).

The aim of this study was to investigate various polymers for use as substitute allograft. The ideal graft would be a composite with similar mechanical characteristics as allograft, and with the ability to form de novo bone.

Methods

High and low molecular weight (MW) forms of three different polymers (polylactic acid (PLA), poly (lactic co-glycolic) acid (PLGA) and polycaprolactone (PCL)) were milled, impacted into discs, and then tested in a custom built shear testing rig, and compared to allograft.

A second stage of the experiment involved the addition of skeletal stem cells (SSC) to each of the milled polymers, impaction, 8 days incubation, and then tests for cell viability and number, via fluorostaining and biochemical (WST-1) assays.


Orthopaedic Proceedings
Vol. 94-B, Issue SUPP_XXXVI | Pages 23 - 23
1 Aug 2012
Tayton E Purcell M Aarvold A Smith J Kalra S Briscoe A Fahmy S Shakesheff K Howdle S Dunlop D Oreffo R
Full Access

Disease transmission, availability and economic costs of allograft have resulted in significant efforts into finding an allograft alternative for use in impaction bone grafting (IBG). Biotechnology offers the combination of skeletal stem cells (SSC) with biodegradable polymers as a potential solution. Recently polymers have been identified with both structural strength and SSC compatibility that offer the potential for clinical translation.

The aim of this study was to assess whether increasing the porosity of one such polymer via super critical CO2 dissolution (SCD) enhanced the mechanical and cellular compatibility characteristics for use as an osteogenic alternative to allograft in IBG.

High molecular weight PLA scaffolds were produced via traditional (solid block) and SCD (porous) techniques, and the differences characterised using scanning electron microscopy (SEM). The polymers were milled, impacted, and mechanical comparison between traditional vs SCD created scaffolds and allograft controls was made using a custom shear testing rig, as well as a novel agitation test to assess cohesion. Cellular compatibility tests for cell number, viability and osteogenic differentiation using WST-1 assays, fluorostaining and ALP assays were determined following 14 day culture with SSCs.

SEM showed increased porosity of the SCD produced PLA scaffolds, with pores between 50-100 micrometres. Shear testing showed the SCD polymer exceeded the shear strength of allograft controls (P<0.001). Agitation testing showed greater cohesion between the particles of the SCD polymer (P<0.05). Cellular studies showed increased cell number, viability and osteogenic differentiation on the SCD polymer compared to traditional polymer (P<0.05) and allograft (P<0.001).

The use of supercritical C02 to generate PLA scaffolds significantly improves the cellular compatibility and cohesion compared to traditional non-porous PLA, without substantial loss of mechanical shear strength. The improved characteristics are critical for clinical translation as a potential osteogenic composite for use in impaction bone grafting.


Orthopaedic Proceedings
Vol. 94-B, Issue SUPP_XXXVI | Pages 20 - 20
1 Aug 2012
Tayton E Fahmy S Aarvold A Smith J Kalra S Briscoe A Purcell M Shakesheff K Howdle S Dunlop D Oreffo R
Full Access

Impaction bone grafting with milled human allograft is the gold standard for replacing lost bone stock during revision hip surgery. Problems surrounding the use of allograft include cost, availability, disease transmission and stem subsidence (usually due to shear failure of the surrounding allograft).

The aim of this study was to investigate various polymers for use as substitute allograft. The ideal graft would be a composite with similar mechanical characteristics as allograft, and with the ability to form de novo bone.

High and low molecular weight (MW) forms of three different polymers (polylactic acid (PLA), poly (lactic co-glycolic) acid (PLGA) and polycaprolactone (PCL)) were milled, impacted into discs, and then tested in a custom built shear testing rig, and compared to allograft.

A second stage of the experiment involved the addition of skeletal stem cells (SSC) to each of the milled polymers, impaction, 8 days incubation, and then tests for cell viability and number, via fluorostaining and biochemical (WST-1) assays.

The shear strengths of both high/ low MW PLA, and high/low MW PLGA were significantly higher than those of milled allograft (P<0.001, P<0.001, P<0.005 and P<0.005) but high and low MW PCL was poor to impact, and had significantly lower shear strengths (P<0.005, P<0.001). Fluorostaining showed good cell survival on high MW PLA, high MW PCL and high MW PLGA. These findings were confirmed with WST-1 assays.

High MW PLA as well as high MW PLGA performed well both in mechanical testing and cell compatibility studies. These two polymers are good contenders to produce a living composite for use as substitute human allograft in impaction bone grafting, and are currently being optimised for this use via the investigation of different production techniques and in-vivo studies.


Orthopaedic Proceedings
Vol. 87-B, Issue SUPP_III | Pages 225 - 225
1 Sep 2005
Yang X Clarke N Sebald W Howdle S Shakesheff K Oreffo R
Full Access

The use of designer scaffolds to deliver biologically active osteogenic growth factors such as recombinant human bone morphogenetic protein-2 (rhBMP-2) to the sites of tissue regeneration in for example orthopaedics, has tremendous therapeutic implications. The aims of this study were to generate biomimetic biodegradable porous osteogenic scaffolds using a supercritical fluid process to encapsulate rhBMP-2, and to examine the ability of the scaffolds to promote human osteoprogenitor differentiation and bone formation in vitro and in vivo.

The rhBMP-2 encapsulated in Poly(-lactic acid) (PLA) scaffolds (100ng/mg PLA) were generated using an innovative supercritical fluid mixing method. The bioactivity of rhBMP-2 encapsulated PLA scaffolds were confirmed by induction of the C2C12 promyoblast cell line into the osteogenic lineage as detected by alkaline phosphatase expression. No induction of alkaline phosphatase-positive cells was observed using blank scaffolds. BMP-2 released from encapsulated constructs promoted adhesion, migration, expansion and differentiation of human osteoprogenitor cells on 3-D scaffolds. Enhanced matrix synthesis and cell differentiation on growth factor encapsulated scaffolds was observed following culture of human osteoprogenitors on explants of chick femoral bone wedge defects in an ex vivo model of bone formation developed using the chick chorioallantoic membrane model. In vivo studies using diffusion chamber implantation and subcutaneous implantation of human osteoprogenitors on rhBMP-2 encapsulated scaffolds showed morphologic evidence of new bone matrix and cartilage formation in athymic mice as assessed by x-ray analysis, immunocytochemistry and birefringence. These studies provide evidence of controlled release of BMP-2 from biodegradable polymer scaffolds initiating new bone formation in vivo.